Technical Data

3200 Innovation Place
Youngstown, Ohio 44509
Phone: (800)523-4899
Fax: (330)797-7543

EMAIL

Weld Brass - Yellow (25 - 40% Zinc) to:

 

Weldability

Electrode
Against

Electrode
Against

Special Information

Magnesium

Very Poor

Copper CL1

Copper CL2

Welding conditions must be accurately controlled

Nickel Alloys

Fair

Copper CL2

Elkonite*
10W3 - CL11

Keep electrodes clean to prevent sticking to the work

Nickel

Fair

Copper CL2

Copper CL2

Keep electrodes clean to prevent sticking to the work.

Stainless Steel

Very Poor

Copper CL2

Elkonite*
10W3 - CL11

 

Chrome Plate

Very Poor

Copper CL2

Elkonite*
10W3 - CL11

 

Cadmium Plate

Poor

Copper CL1

Elkonite*
10W3 - CL11

Keep electrodes clean to prevent sticking to the work.

Galvanized Iron
Zinc Plate

Poor

Copper CL1

Elkonite*
10W3 - CL11

Keep electrodes clean to prevent sticking to the work.

Terne Plate

Poor

Copper CL1

Elkonite*
10W3 - CL11

Keep electrodes clean to prevent sticking to the work.

Tin Plate

Poor

Copper CL1

Elkonite*
10W3 - CL11

Keep electrodes clean to prevent sticking to the work.

C.R. Steel

Poor

Copper CL2

Elkonite*
10W3 - CL11

Low weld strength. No actual nugget occurs, a “stick” is obtained.

Phosphor Bronze

Good

Copper CL2

Elkonite*
10W3 - CL11

Good weld strength

Silicon Bronze

Good

Copper CL2

Elkonite*
10W3 - CL11

Good weld strength

Nickel Silver

Good

Copper CL2

Elkonite*
10W3 - CL11

Good weld strength

Cupro Nickel

Good

Copper CL2

Elkonite*
10W3 - CL11

 

Brass - Yellow

Good

Copper CL2

Copper CL2

Good weld strength